1. Blister Edge Cracking

Root causes

  • Deep draw design with sharp corners and insufficient fillet radius; stress concentrates on sharp edges after forming.

  • Wrong material selection: brittle materials such as general PS are used for deep-draw parts.

  • Improper sheet heating: overheating or under-heating makes the plastic sheet lose ductility.

  • Excessive demoulding force or fast ejection speed.

Prevention measures

  • Add rounded corners on all sharp transitions; avoid 90-degree sharp corners for deep cavities.

  • Switch to flexible materials like APET, PETG or PP for deep-draw blisters instead of ordinary PS.

  • Calibrate oven temperature and heating time according to material thickness.

  • Adjust demoulding speed and add proper draft angle on moulds.


2. Blister-Card Delamination (Heat Seal Failure)

Root causes

  • Unmatched heat-seal coating on paper card and blister plastic material.

  • Incorrect heat sealing parameters: temperature too low, insufficient pressure or short dwell time.

  • Oil, dust or release agent contaminates the sealing area.

  • High temperature and humidity during long sea transport weaken the seal bond.

Prevention measures

  • Confirm the coating type of paper card before production; match the coating with your blister material (PET / PVC / PP).

  • Run heat seal parameter tests with actual sheets and paper cards before mass run.

  • Keep the sealing surface clean and avoid release agent contamination.

  • Perform heat & humidity aging tests on sealed samples to simulate ocean shipping conditions.


3. Webbing / Stringing Between Cavities

Root causes

  • Too narrow spacing between adjacent cavities.

  • Excessive sheet heating, the plastic becomes overly soft and sags easily.

  • Improper vacuum timing: vacuum pulls too fast before the sheet is fully formed.

Prevention measures

  • Keep reasonable gap between cavities at the design stage.

  • Reduce heating time if the sheet sags heavily.

  • Tune vacuum sequence: slow down initial vacuum pull for multi-cavity moulds.


4. Surface Scratches and Wavy Marks

Root causes

  • Poor mould surface polishing, texture or machining marks transfer to blisters.

  • Dust and hard particles on the sheet, mould or conveyor chain.

  • Sheet quality defect: inconsistent thickness or raw material impurities.

Prevention measures

  • Polish mould surface to required finish before sampling and mass production.

  • Maintain a clean forming workshop, regularly clean mould and conveying system.

  • Inspect incoming plastic sheets for waves, spots and impurities before use.


5. Rattling & Loose Product Inside Blister Cavity

Root causes

  • Cavity contour only follows the outer outline of the product, without positioning ribs or limit structure.

  • Tolerance mismatch: blister cavity is much larger than the finished product.

  • Shrinkage after thermoforming is not considered during design.

Prevention measures

  • Add positioning ribs, stop points or contour bosses to hold the item tightly.

  • Calculate thermoforming shrinkage rate when drawing cavity dimensions.

  • Test fit samples with your actual finished product before mould fabrication.


Practical Sourcing Tip for Buyers

Many defects only appear after long ocean shipment, not right after production. We highly recommend you arrange reliability tests on pre-production samples: store sealed blister packs under high temperature and high humidity conditions for a period, then run drop test and seal strength test. This step helps you catch hidden risks before mass shipment.


Conclusion

Blister defects rarely come from a single factor. They are usually the combined result of design, material, mould and machine parameter issues. Early communication between your product team and blister manufacturer can avoid most quality headaches.

If you need custom blister trays, clamshells or carded blister packs with stable quality and EU compliance support, feel free to contact us for free samples and technical consultation.


CONTACT US

Add:No.896,S358 provincial road,Sha- tou Community, Chang'an Town, Dongguan, Guangdong,China 523869

Tel: +86 136 5260 3312

WhatsApp: +852 6090 8972

E-mail: sales02@angzhan.com.cn

WRITE US

Copyright © Dongguan Coniro Tech Co., Ltd. All Rights Reserved | Sitemap